Dpm

Discussion in 'Subfloor Preparation' started by Mark Higgins, May 11, 2019.

  1. Mark Higgins

    Mark Higgins Member

    11
    0
    1
    Hi guys
    Abit of advice plz
    Calcium sulphate screed needing a dpm what's the options out there at the minute?
    Only taken a non invasive reading at the minute obviously the results are all over the place David wilson house I use to work for a contractor who used uzin gold on the David Wilson homes but I'm not 100% confident with that at all.
     
  2. dazlight

    dazlight Super Moderator

    6,839
    1,615
    113
    Has it UFH?
     
  3. Mark Higgins

    Mark Higgins Member

    11
    0
    1
  4. Spacey

    Spacey Super Moderator Staff Member

    6,516
    1,878
    113
    Best not to DPM let it dry out its fast drying or force dry with UFH if it has any
    Grind laitence prime and use a gypsum based smoothing compound let that dry for 48 hours and use a HT wet set adhesive not PS
     
  5. dazlight

    dazlight Super Moderator

    6,839
    1,615
    113
    Uzin do a system Mark I think only when the floor is under 90%RH
    I did it on a job last year. PE425, PE404, PE280 , NC110
     
  6. Distinctive Adam

    Distinctive Adam Well-Known Member

    1,688
    496
    83
    Murexin IH16, msx-3, d4, ca20.
     